ASTM, ISO & GB Test Methods

Tarpaulin Test Standards

Tarpaulin test standards are the named methods — ASTM D751, ISO 13934-1, ISO 1421-1 and others — that define how a cover’s tensile strength, tear strength, GSM, UV resistance and flame retardancy are measured. A test value is only as useful as the method behind it.

Standard Families

What Tarpaulin Test Standards Apply?

A tarpaulin is a coated fabric, so the relevant tarpaulin testing standards fall into two families. The first covers coated fabrics specifically. The second covers textiles generally, and is applied to the base fabric before or after coating. Knowing which family a report cites tells you whether the supplier is testing the finished product or a proxy for it.

01 / MATERIAL TYPE

Material Decides the Family

ISO 13934-1 is written for woven and knitted textiles. ISO 1421-1 is written for rubber- and plastic-coated fabrics, which is what a PVC tarpaulin actually is. Both measure tensile strength, but the specimen and conditioning differ, and the values are not interchangeable.

02 / COATED FABRIC

Testing the Finished Cover

ASTM D751 (Section 11) and ISO 1421-1 operate directly on the coated fabric, so the result describes the product that arrives — not the greige roll it was made from.

03 / TEXTILE BASE

Testing the Raw Material

ISO 13934-1 and ASTM D5034 are usually run as a check on the woven base fabric before coating. Reading a textile value as a coated-fabric value compares two different things.

Principal Test Standards for Tarpaulins
Property Primary Standard What It Measures
Tensile Strength (Coated Fabric) ISO 1421-1; ASTM D751 (Section 11) Breaking force in N/5cm, warp and weft
Tensile Strength (Textile) ISO 13934-1; ASTM D5034 (grab) Breaking force and elongation at break
Tear Strength ASTM D751 (Section 31); ASTM D4533; ASTM D1424; ISO 4674-1 Resistance to tear propagation
Weight / GSM ISO 3801 Mass per unit area in g/m²
UV / Weathering ISO 4892-2 (xenon arc); ASTM G53 Strength retention after exposure hours
Water Resistance GB/T 4744 Hydrostatic resistance
Flame Retardancy GB/T 5455 Flammability behaviour

A report that names the right family for the product is a first signal that the testing was done properly. Values taken under a textile method cannot be read as coated-fabric values, and vice versa.

On smaller screens, scroll horizontally to view all columns.

Two Families, One Question

ISO 13934-1 is written for woven and knitted textiles. ISO 1421-1 is written for rubber- and plastic-coated fabrics — which is what a PVC tarpaulin actually is. Both measure tensile strength; the values are not interchangeable.

Name the Method on the Report

We test both woven HDPE tape coated with LDPE and polyester scrim coated with PVC, and we name the method on each report. Ask which family your specification cites before comparing numbers.

Force in N/5cm, Warp & Weft

Tarpaulin Tensile Strength Test Standards (N/5cm)

Tensile strength is the force a tarpaulin resists before it breaks under a straight pull. It is quoted in N/5cm — newtons per 5 centimetres of fabric width — and must be measured in both directions: warp (along the roll) and weft (across it).

Tensile Strength Methods Compared Which standard applies depends on whether the specimen is coated fabric or textile base cloth. Scroll horizontally on smaller screens.
Standard Applies To Test Procedure
ASTM D751 (Section 11) Coated fabric Grab test or cut strip test
ISO 1421-1 Coated fabric Strip method
ISO 13934-1 Textile base fabric Strip method
ASTM D5034 Textile base fabric Grab method

ASTM D751 and ISO 1421-1 are the coated-fabric methods used on the finished tarpaulin. ISO 13934-1 and ASTM D5034 are textile methods applied to the woven base fabric.

Reference Tensile Strength by Grade Company-reported figures for the grades we run. Verify against the batch test report for your order.
Grade or Requirement Reference (N/5cm) Note
120 GSM PE ≈ 400 Company-reported value
180 GSM PE ≈ 650 Company-reported value
Relief-sector minimum 500–600 Typically required in both directions

As a rule, a heavier grade holds more force. The relief-sector floor of 500–600 N is why a serious buyer asks for the report rather than the adjective.

Company-reported figures — verify per batch. Values attach to the grade, not to the material family. Confirm the standard name, the direction tested and the unit on the batch report before comparing suppliers.

01 / DIRECTION

Warp and Weft Both Matter

A single-direction figure is an incomplete specification. Wind load and tensioning do not distinguish between the two axes of the fabric.

02 / UNIT

N/5cm, Not N or kgf

The standard specimen width is 5 cm. If the unit on a catalogue figure does not match, the number cannot be compared directly with a test report.

03 / GRADE

The Value Lives on the Grade

A 120 GSM PE tarpaulin tests at roughly 400 N/5cm; 180 GSM climbs toward 650 N/5cm. The same fabric family can carry very different numbers.

Once the Cut Has Started

Tarpaulin Tear Strength Test Standards

Tensile strength tells you what a tarpaulin resists under a straight, even pull. Tear strength tells you what happens once a puncture or a cut has already started — which is how tarpaulins actually fail in the field.

Where Failure Begins Eyelets & Hems

A snag on a bolt, a sharp edge on a load, or an over-tensioned eyelet starts a tear. Tear strength decides whether it stops or runs.

ASTM D4533
Trapezoid tear
ASTM D1424
Elmendorf tear
ISO 4674-1
Coated-fabric tear
Rope-reinforced hem
Spreads load at fixings
METHOD 01

ASTM D4533

Trapezoid specimen Pulled from a known starting point

Trapezoid Tear Measures how a started tear propagates
METHOD 02

ASTM D1424

Pendulum apparatus Applied to an already-started tear

Elmendorf Tear Force required to continue a tear
METHOD 03

ISO 4674-1

Coated-fabric specimen Named on European specifications

Coated-Fabric Tear Most often cited by relief tenders

Test the Fabric — and Specify the Finishing

Tear strength matters most exactly where covers fail first: at the eyelets and the hems. A rope-reinforced hem spreads the load at the fixing points, which is what keeps a tear from starting there in the first place. The fabric’s tear strength and the finishing detail work together — test the fabric, but specify the finishing too.

Tear results are reported in newtons or grams-force depending on the method, and the methods are not interchangeable. Confirm which tear test your specification names, and that the finishing detail has been agreed separately.

Beyond Tensile & Tear

GSM, UV, Water Resistance and Flame Retardancy Standards

Tensile and tear are the headline tests, but a complete tarpaulin test report covers the properties that decide service life and compliance.

01 / WEIGHT

GSM Is Tested by ISO 3801

A measured area of fabric is weighed under controlled conditions. This is the figure buyers use to compare grades — and the one most often wrong on arrival.

02 / WEATHERING

UV Is Tested by ISO 4892-2

A specimen is exposed to a xenon arc lamp that simulates sunlight, then tested for how much tensile strength remains after a defined number of hours.

03 / COMPLIANCE

Water and Flame Are Measured

GB/T 4744 measures hydrostatic pressure. GB/T 5455 measures burning behaviour. Both are a method and a result, not an adjective.

Standards by Property
Property Standard What It Measures
GSM (Weight) Grams per square metre ISO 3801 Mass per unit area in g/m². Tested on a measured area rather than stated from the label.
UV / Weathering Strength retention ISO 4892-2 (xenon arc) ASTM G53 Tensile strength retained after a defined number of exposure hours. The honest way to state “UV resistant”.
Water Resistance Hydrostatic head GB/T 4744 Water pressure, in millimetres of water column, a fabric withstands before water passes through.
Flame Retardancy Burning behaviour GB/T 5455 How quickly a flame spreads and whether the fabric self-extinguishes.

Each property has a named method behind it. A claim without a method and a result is not a specification. Scroll horizontally on smaller screens.

How to Read a UV Claim
Item Typical Requirement What It Means
Exposure method ISO 4892-2 xenon arc Simulated sunlight
Test hours 1,500 hours Common on relief-sector specifications
Strength retention ≥ 80% Tensile strength remaining after exposure

UV and flame treatments are covered under special treatments. Confirm the method, the hours and the retention figure in writing.

GSM Is the Figure Most Often Wrong on Arrival

Testing GSM to a named method — rather than stating it from the label — is what makes it a specification instead of a claim. Compare grades in g/m², not by feel.

Nothing Here Is Fireproof

A flame-retardant tarpaulin is tested for burning behaviour — how quickly a flame spreads and whether it self-extinguishes. The test measures how the fabric behaves under a controlled flame, not the word “fireproof”.

From Claim to Checkable Number

How to Read a Batch Test Report

The batch test report is where all of the above becomes something you can act on. It is the document that should turn “trust me” into “here is the number for your batch”.

It Names the Batch

The report must state the grade and batch number it applies to, so it can be traced to a specific production run rather than to a marketing sample.

It Names the Method

Each line carries the standard name and number — not just the property. A value without a method is a number with no provenance.

It Names Direction and Unit

Tensile and tear carry warp and weft figures. Every line carries its unit: N/5cm, g/m², hours or millimetres of water column.

Batch Traceability Tied to Your Batch

A report that cannot be tied to a specific batch cannot protect you from the sample-versus-container mismatch that is every importer’s real fear.

01 / METHOD AND BATCH

Ask for the Method, Not the Claim

A report that omits the method, the batch number or the direction is not a report you can rely on. Method, value and batch have to sit together on the same page.

02 / VERIFICATION

Ask for the Report, Not the Brochure

We run a 26-stage quality control system from incoming material through to pre-shipment inspection, and we offer the batch test report for every order. The methods are run in-line and at final inspection — not once for a marketing document.

Tarpaulin Testing Questions

Frequently Asked Questions

Answers about test methods, batch reports, coated-fabric versus textile standards, and how to verify a claim.

What test standards apply to tarpaulin?

The main tarpaulin test standards are ASTM D751 for coated fabrics, ISO 13934-1 and ASTM D5034 for textile tensile strength, ISO 1421-1 for coated-fabric tensile strength, ASTM D4533 and ASTM D1424 for tear strength, ISO 3801 for GSM, and ISO 4892-2 for UV weathering.

Which standard applies depends on the material and the market.

What does ASTM D751 measure?

ASTM D751 is the standard test methods for coated fabrics. It covers tensile strength, elongation, tear strength, adhesion and weathering for fabrics such as tarpaulins.

It is the primary ASTM method used for tarpaulin testing in the US market.

What is the difference between ISO 13934-1 and ISO 1421-1?

ISO 13934-1 is a textile standard for determining breaking force in woven and knitted fabrics. ISO 1421-1 is the equivalent standard for rubber- and plastic-coated fabrics, which is what a PVC tarpaulin is.

Both measure tensile strength, but the specimen and conditioning differ, and the values are not interchangeable.

How is tarpaulin tensile strength measured?

Tarpaulin tensile strength is measured by pulling a specimen in a testing machine until it breaks, and recording the force in N/5cm. It is tested in both the warp and weft directions.

ASTM D751 uses a grab or cut strip test; ISO 1421-1 uses a strip method for coated fabric.

How do I know if a batch test report is genuine?

A genuine batch test report names the grade and batch number, the test method for each line, the measured value with its unit, the direction tested, and the laboratory and date.

A report missing the method, the batch number or the direction should not be relied on.

What UV test standard applies to tarpaulin?

ISO 4892-2 is the xenon arc method most often used to test tarpaulin UV resistance. It exposes the fabric to simulated sunlight and measures the tensile strength retained after a defined number of hours.

A typical relief specification requires at least 80% retention after 1,500 hours.

Choose a Tarpaulin You Can Verify

Tensile and tear tell you how the fabric behaves under load and once damaged. GSM tells you what you are paying for per square metre. UV hours tell you how long it will hold up in the sun. Read together in a genuine batch test report, they let you defend the specification to your own customer without re-testing every delivery. Send the intended application, the GSM and the destination port, and we will return a specification, a sample plan and a landed-cost estimate.

Request a Sample Test Report

Tell us what you need

Share your material, dimensions, quantity and destination. Our team will help with your specification.

Contact Form